PCC Admixtures
Reviewed by licensed engineers
Checked against its sources by licensed professional engineers on the previous site, where reviewers weren’t recorded by name.
Admixtures are the ingredients in PCC other than aggregate, portland cement and water. Typically, an admixture is added to alter a specific PCC property such as workability, setting time, strength or durability.
| Type | Desired Effect | Material |
|---|---|---|
| Accelerators | Accelerate setting and early strength development | Calcium chloride, triethanolamine, sodium thiocyanate, calcium formate, calcium nitrite, calcium nitrate |
| Air detrainers | Decrease air content | Tributyl phosphate, dibutyl phthalate, octyl alcohol, water-insoluble esters of carbonic and boic acid, silicones |
| Air-entraining | Improve durability in environments of freeze-thaw, deicers, sulfate and alkali reactivityImprove workability | Salts of wood resins, lignin, petroleum acids, proteinaceous material or sulfonated hydrocarbonsSome synthetic detergentsFatty and resinous acids and their saltsAlyklbenzene sulfonates |
| Alkali-reactivity reducers | Reduce alkali-reactivity expansion | Pozzolans, blast-furnace slag, salts of lithium and barium, air-entraining agents |
| Bonding | Increase bond strength | Rubber, polyvinyl chloride, polyvinyl acetate, acrylics, butadienestyrene copolymers |
| Corrosion inhibitors | Reduce steel corrosion activity in a chloride environment | Calcium nitrite, sodium nitrite, sodium benzoate, certain phosphates or flurosilicates, fluroaluminates |
| Damp proofing | Retard moisture penetration into dry PCC | Soaps of calcium or ammonium stearate or oleateButyl stearatePetroleum products |
| Cementitious Minerals | Hydraulic propertiesPartial cement replacement | Ground granulated blast-furnace slagNatural cementHydraulic hydrated lime |
| Natural pozzolans | Pozzolonic activityImprove workability, plasticity, sulfate resistanceReduce alkali reactivity, permeability, heat of hydrationPartial cement replacementFiller | Diatomaceous earth, opaline cherts, clays, shales, volcanic tuffs, pumicitesFly ash (classes C and F)Silica fume |
| Inert minerals | Improve workabilityFiller | Marble, dolomite, quartz, granite |
| Permeability reducers | Reduce permeability | Silica fume, fly ash, ground slag, natural pozzolans, water reducers, latex |
| Pumping aids | Improve pumpability | Organic and synthetic polymersOrganic flocculentsOrganic emulsions of paraffin, coal tar, asphalt, acrylicsBentonite and pyrogenic silicasNatural pozzolansFly ashHydrated lime |
| Retarders | Retard setting time | Lignin, borax, sugars, tartaric acid and salts |
| Superplasticizers (high-range water reducers) | Reduce water-cement ratio by a minimum of 12%Increase workability at low water-cement ratios | Sulfonated melamine formaldehyde condensatesSulfonated naphthalene formaldehyde condensatesLignosulfonates |
| Water reducer | Reduce water demand by a minimum of 5% | LignosulfonatesHydroxylated carboxylic acidsCarbohydrates |
| Workability agents | Improve workability | Air-entraining admixturesCementitious materials, natural pozzolans and inert minerals (except silica fume) |
Teaching this? Figures and worked examples are free to use with credit. How to cite
Cite this page
APA
Pavement Interactive. (2018, August 1). PCC admixtures. HeadLight. Retrieved [the date you read it], from https://pavementinteractive.org/reference-desk/design/mix-design/pcc-admixtures/
ASCE
Pavement Interactive. (2018). “PCC Admixtures.” HeadLight, <https://pavementinteractive.org/reference-desk/design/mix-design/pcc-admixtures/> ([the date you read it]).
BibTeX
@misc{pavint-pcc-admixtures,
author = {{Pavement Interactive}},
title = {PCC Admixtures},
year = {2018},
publisher = {HeadLight},
howpublished = {\url{https://pavementinteractive.org/reference-desk/design/mix-design/pcc-admixtures/}},
note = {Accessed [date]}
}