# Sampling Asphalt Binders and Emulsions

How asphalt binders and emulsions are sampled from tanks, transports and distributors, which containers to use, and how to avoid contaminating the sample.

- Canonical URL: https://pavementinteractive.org/reference-desk/testing/sampling/sampling-asphalt-binders-and-emulsions/
- Last updated: 2026-11-01
- Standards: AASHTO R 66, ASTM D140

Performance grading tests on [asphalt binder](https://pavementinteractive.org/glossary/asphalt-binder/) are sensitive: a small amount of solvent, a little overheating, or the wrong container can change a binder's grade. Sampling binder is less about representing a variable material, since a well-mixed tank is fairly uniform, and more about getting the binder from the tank to the laboratory unchanged. The national practice is AASHTO R 66 (ASTM D140), which replaced the older T 40 (California Department of Transportation, 2022[^1]).

## Where Binder Is Sampled

- **Supplier terminal or refinery.** Agencies that certify suppliers sample at the terminal tank to verify the grade.
- **Transport on arrival.** A sample taken from the delivery tanker at the plant or job checks what was delivered.
- **Plant tank or feed line.** A sample from the line feeding the mixer checks the binder actually used in production, after any blending or additives at the plant.
- **Distributor truck.** For chip seals, tack coats and other sprayed treatments, the distributor is sampled from its sampling valve.

Most tanks and transports have a dedicated sampling valve. Before taking the sample, the valve is opened and a quantity of binder is drawn off and discarded, to clear material that has been sitting in the line. Samples are never dipped from an open hatch with a container that has been in contact with anything else (California Department of Transportation, 2022[^1]).

## Containers

- **Asphalt binders** are sampled into new, clean, unlined metal cans with tight lids, usually about 1 L (1 quart). Cans are not washed with solvent and not reused.
- **Emulsions** are sampled into clean, wide-mouth plastic containers with screw caps. They are not put in metal cans, which can corrode and break the emulsion, or in glass.
- **Cutbacks** follow the binder practice but need tight seals because their solvents evaporate.

Containers are filled nearly full, sealed at once, and wiped clean on the outside with a dry cloth, never with solvent. Each is labeled on the body, not the lid, with the grade, supplier, tank or transport, date, time and sampler (California Department of Transportation, 2022[^1]).

## Handling

- Emulsions must not freeze, and should be tested within the time the specification allows, because they can settle or break in storage.
- Binder samples are not repeatedly reheated. Each reheating ages the binder and can push it toward a stiffer grade. Laboratories heat a sample once and pour all the test specimens they need at that time.
- Samples are protected from contamination by dust, water or oil during transport.

## Related Articles

- [Superpave Performance Grading](https://pavementinteractive.org/reference-desk/materials/asphalt/superpave-performance-grading/)
- [Emulsified Asphalt](https://pavementinteractive.org/reference-desk/materials/asphalt/emulsified-asphalt/)
- [Asphalt Safety](https://pavementinteractive.org/reference-desk/materials/asphalt/asphalt-safety/)

## Standard Practices

- AASHTO R 66, ASTM D140: Sampling asphalt materials

## Sources

[^1]: California Department of Transportation (Caltrans) (2022). Method of Test for Sampling Highway Materials and Products Used in the Roadway Pavement Structure Sections (California Test 125). Transportation Laboratory, California Department of Transportation. Sacramento, CA. https://dot.ca.gov/-/media/dot-media/programs/engineering/documents/californiatestmethods-ctm/ct-125-aug2022-a11y.pdf