# Dowel Bars

Dowel bars are short steel bars that provide a mechanical connection between slabs without restricting horizontal joint movement.

- Canonical URL: https://pavementinteractive.org/reference-desk/pavement-types-and-history/pavement-types/dowel-bar/
- Last updated: 2026-11-01

Dowel bars are short steel bars that provide a mechanical connection between slabs without restricting horizontal joint movement. They increase load transfer efficiency by allowing the leave slab to assume some of the load before the load is actually over it. This reduces joint deflection and stress in the approach and leave slabs.

![](https://pavementinteractive.org/wp-content/uploads/2021/06/IMGP4601-scaled.jpg)

*Figure 1.* Dowel bars (purple steel bars) being placed at the location where transverse joints will be in the finished PCC pavement. Here, bars are attached to "cages", which are minimalist bar structures designed to hold dowels at the right location before the concrete is paved over them. The cages perform no function other than initial alignment assistance.

Dowel bars are typically 32 to 38 mm (1.25 to 1.5 inches) in diameter, 460 mm (18 inches) long and spaced 305 mm (12 inches) apart. Specific locations and numbers vary by state, however a typical arrangement might look like Figure 1. In order to prevent corrosion, dowel bars are either coated with stainless steel (Figure 2) or epoxy (Figure 3). Dowel bars are usually inserted at mid-slab depth and coated with a bond-breaking substance to prevent bonding to the PCC. Thus, the dowels help transfer load but allow adjacent slabs to expand and contract independent of one another. Figure 3 shows typical dowel bar locations at a transverse [construction joint](https://pavementinteractive.org/glossary/construction-joint/).

![Stainless steel-clad dowel bars/ (Epoxy Coating on Ends Only](https://pavementinteractive.org/wp-content/uploads/2008/06/Dowel_bars21.jpg)

![Dowel bars in place at a construction joint- the green color is from the epoxy coating.](https://pavementinteractive.org/wp-content/uploads/2008/06/Dowel_bars11.jpg)

*Figures 2 and 3.* Stainless steel-clad dowel bars/ (Epoxy Coating on Ends Only) Dowel bars in place at a construction joint- the green color is from the epoxy coating.

## Why Dowels Are Used

Some [load transfer](https://pavementinteractive.org/reference-desk/pavement-types-and-history/pavement-types/load-transfer/) across a transverse joint comes from [aggregate interlock](https://pavementinteractive.org/glossary/aggregate-interlock/) between the two slabs, but heavy truck loads raise the stresses at slab edges beyond what aggregate interlock can carry, and interlock stops working if slab movement opens the joint. Dowel bars carry the load across the joint in either case and help prevent [faulting](https://pavementinteractive.org/reference-desk/pavement-management/pavement-distresses/faulting/). They are used in new construction and in rehabilitation such as slab replacement, and they can be [retrofitted](https://pavementinteractive.org/reference-desk/maintenance-and-rehabilitation/rehabilitation/dowel-bar-retrofit/) into existing pavements built without them.

## Placement

- **New construction.** Dowels are usually set in advance in baskets, simple wire frames that hold the bars at the correct height, at each future transverse joint; the joint is [sawed](https://pavementinteractive.org/reference-desk/construction/placement/sawcutting/) afterward. With [slipform paving](https://pavementinteractive.org/reference-desk/construction/placement/slipform-paving/), a dowel bar inserter attached to the paver can instead place the bars in the fresh concrete. See [Dowel Bar Placement](https://pavementinteractive.org/reference-desk/construction/placement/dowel-bar-placement/).
- **Slab replacement.** Holes are drilled into the face of the adjacent slab, often with automated equipment that drills several holes at once, and the dowels are inserted before the replacement slab is cast. Where several consecutive slabs are replaced, the joints between them can use baskets as in new construction.
- **Retrofit.** A slot is cut at each dowel location, cleaned of debris, and the bar is set in a chair that holds it in position and alignment; the slot is then filled with quick-setting cementitious grout, and the surface is usually [diamond ground](https://pavementinteractive.org/reference-desk/maintenance-and-rehabilitation/maintenance/diamond-grinding/). See [Dowel Bar Retrofit Procedures](https://pavementinteractive.org/reference-desk/pavement-types-and-history/pavement-types/dowel-bar-retrofit-procedures/).

## Materials

Because dowels must last as long as the pavement, corrosion resistance is a key consideration where they are exposed to moisture and deicing chemicals. Dowels range from plain, uncoated steel to solid stainless steel, and the more corrosion-resistant types generally cost more. High-chromium steel, with more chromium than ordinary steel but less than stainless steel, is a popular choice because it resists corrosion well at a much lower cost than stainless. Whatever the material, dowels are coated with a bond breaker so the slabs can move horizontally while the bar continues to transfer load.

**Table 1.** Table showing dowel bar types in order from most corrosion-resistant to least.

| Most corrosion resistance, highest cost |
| --- |
| Solid stainless steel |
| Stainless steel clad |
| Stainless steel sleeve, epoxy-coated insert |
| High chromium steel |
| Zinc clad |
| Epoxy-coated steel |
| Plain, uncoated steel |
| Least corrosion resistance, lowest cost |

## Spacing and Alignment

Dowels are normally placed at mid-depth of the slab. Across the lane they are typically spaced 305 mm (12 inches) apart, with the first bar 305 mm (12 inches) from the slab edge; a bar closer to the edge can itself create stresses that [damage the slab](https://pavementinteractive.org/reference-desk/pavement-management/pavement-distresses/joint-load-transfer-system-deterioration/). In retrofits, dowels are commonly placed only in the wheelpaths to reduce the number of slots cut.

## Surveys

### Dowel Bar Survey

#### Questions

- Do you utilize epoxy coated smooth dowels in your concrete pavements?
- Have you excavated smooth dowels from concrete pavements recently? If yes, what condition were they in generally?
- Have you experienced rusting problems with epoxy coated smooth dowels? If yes, about how long were they in place and was the rusting cause for pavement joint failure?
- Do you use smooth dowels that are not epoxy coated? If yes, what coatings do you use and what percentage of your smooth dowels are coated with something other than epoxy?
- Additional comments:
- Would you like a coy of the compiled results of this survey?

#### Results

[Dowel Bar Survey](https://pavementinteractive.org/wp-content/uploads/2008/06/DowelBar1.pdf)

### Epoxy Coated Dowel Bars Used in Portland Cement Concrete Pavements-Kentucky DOT

#### Questions

- Do you utilize epoxy coated smooth dowels in your concrete pavements?
- Have you excavated smooth dowels from concrete pavements recently? If yes, what condition were they in generally?
- Have you experienced rusting problems with epoxy coated smooth dowels? If yes, about how long were they in place and was the rusting cause for pavement joint failure?
- Do you use smooth dowels that are not epoxy coated? If yes, what coatings do you use and what percentage of your smooth dowels are coated with something other than epoxy?

#### Results

[Epoxy Coated Dowel Bars Used in Portland Cement Concrete Pavements](https://pavementinteractive.org/wp-content/uploads/2008/06/DowelBarKDOTSurvey1.pdf)