# Viscosity Grading

In the early 1960s an improved asphalt grading system was developed that incorporated a rational scientific viscosity test. This scientific test replaced the empirical penetration test as the key asphalt binder characterization.

- Canonical URL: https://pavementinteractive.org/reference-desk/materials/asphalt/viscosity-grading/
- Last updated: 2018-07-27
- Review: reviewed by licensed professional engineers on the previous Pavement Interactive site, where reviewers were not recorded by name
- Standards: AASHTO T 201, ASTM D2170, AASHTO M 226, ASTM D3381

In the early 1960s an improved asphalt grading system was developed that incorporated a rational scientific viscosity test. This scientific test replaced the empirical penetration test as the key [asphalt binder](https://pavementinteractive.org/glossary/asphalt-binder/) characterization. Viscosity grading quantifies the following asphalt binder characteristics:

- Viscosity at 60°C (140°F)
- Viscosity at 135°C (275°F)
- Penetration depth of a 100 g needle applied for 5 seconds at 25° C (77° F)
- Flash point temperature
- Ductility at 25°C (77°F)
- Solubility in trichloroethylene
- Thin-film oven test (accounts for the effects of short-term aging):

  - Viscosity at 60° C (140° F)
  - Ductility at 25° C (77° F)

Viscosity grading can be done on original (as-supplied) asphalt binder samples (called AC grading) or aged residue samples (called AR grading). The AR viscosity test is based on the viscosity of aged residue from the rolling thin film oven test. With AC grading, the asphalt binder is characterized by the properties it possesses before it undergoes the HMA manufacturing process. The AR grading system is an attempt to simulate asphalt binder properties after it undergoes a typical HMA manufacturing process and thus, it should be more representative of how asphalt binder behaves in HMA pavements. Table 1 lists key advantages and disadvantages of the viscosity grading system.

**Table 1.** Advantages and Disadvantages of Viscosity Grading (from Roberts et al., 1996)

| Advantages | Disadvantages |
| --- | --- |
| Unlike penetration depth, viscosity is a fundamental engineering parameter. | The principal grading (done at 25° C (77° F)) may not accurately reflect low-temperature asphalt binder rheology. |
| Test temperatures correlate well with: - 25° C (77° F) – average pavement temp. - 60° C (140° F) – high pavement temp. - 135° C (275° F) – HMA mixing temp. | When using the AC grading system, thin film oven test residue viscosities can vary greatly with the same AC grade. Therefore, although asphalt binders are of the same AC grade they may behave differently after construction. |
| Temperature susceptibility (the change in asphalt binder rheology with temperature) can be somewhat determined because viscosity is measured at three different temperatures (penetration only is measured at 25° C (77° F)). | The testing is more expensive and takes longer than the penetration test. |
| Testing equipment and standards are widely available. |  |

Viscosity is measured in poise (cm-g-s = dyne-second/cm², named after Jean Louis Marie Poiseuille). The lower the number of poises, the lower the viscosity and thus the more easily a substance flows. Thus, AC-5 (viscosity is 500 ± 100 poise at 60° C (140° F)) is less viscous than AC-40 (viscosity is 4000 ± 800 poise at 60° C (140° F)). Table 2 shows standard viscosity grades for the AC and AR grading systems from AASHTO M 226 and ASTM D 3381. Typical grades used for HMA paving in the U.S. are AC-10, AC-20, AC-30, AR-4000 and AR 8000.

**Table 2.** AASHTO M 226 and ASTM D 3381 Viscosity Grades

| Standard | Grading based on Original Asphalt (AC) |  |  |  |  |  | Grading based on Aged Residue (AR) |  |  |  |  |
| --- | --- | --- | --- | --- | --- | --- | --- | --- | --- | --- | --- |
| AASHTO M 226 | AC-2.5 | AC-5 | AC-10 | AC-20 | AC-30 | AC-40 | AR-10 | AR-20 | AR-40 | AR-80 | AR-160 |
| ASTM D 3381 | AC-2.5 | AC-5 | AC-10 | AC-20 | AC-30 | AC-40 | AR-1000 | AR-2000 | AR-4000 | AR-8000 | AR-16000 |

### Kinematic Viscosity

The kinematic viscosity of a liquid is the absolute (or dynamic) viscosity divided by the density of the liquid at the temperature of measurement. The 135° C (275° F) measurement temperature was chosen to simulate the mixing and [laydown](https://pavementinteractive.org/glossary/laydown/) temperatures typically encountered in HMA pavement construction.

The basic kinematic viscosity test measures the time it takes for a fixed volume of asphalt binder to flow through a capillary viscometer under closely controlled conditions of head and temperature (ASTM, 2001[^1]).

## Standard Test Methods

- AASHTO T 201 and ASTM D 2170: Kinematic Viscosity of Asphalts ([Bitumens](https://pavementinteractive.org/glossary/bitumens/))

## Sources

[^1]: American Society for Testing and Materials (ASTM) (2001). Annual Book of ASTM Standards, Section four: Construction. vol. 4.03. American Society for Testing and Materials. West Conshohocken, PA.