# Introduction to Aggregate

Aggregate" is a collective term for the mineral materials such as sand, gravel and crushed stone that are used with a binding medium (such as water, bitumen, portland cement, lime, etc.) to form compound materials (such as asphalt…

- Canonical URL: https://pavementinteractive.org/reference-desk/materials/aggregate/introduction/
- Last updated: 2026-11-01
- Standards: ASTM D1073, ASTM D242, ASTM D692

Aggregate" is a collective term for the mineral materials such as sand, gravel and crushed stone that are used with a binding medium (such as water, bitumen, [portland cement](https://pavementinteractive.org/glossary/portland-cement/), lime, etc.) to form compound materials (such as [asphalt concrete](https://pavementinteractive.org/glossary/asphalt-concrete/) and portland cement concrete). By volume, aggregate generally accounts for 92 to 96 percent of HMA and about 70 to 80 percent of portland cement concrete. Aggregate is also used for base and subbase courses for both flexible and [rigid pavements](https://pavementinteractive.org/glossary/rigid-pavement/).

Aggregates can either be natural or manufactured. Natural aggregates are generally extracted from larger rock formations through an open excavation (quarry). Extracted rock is typically reduced to usable sizes by mechanical crushing. Manufactured aggregate is often the byproduct of other manufacturing industries.

This section will briefly discuss aggregate sources and quarrying operations then describe the basic aggregate mineral, chemical and physical properties most important to pavements and the typical tests used to determine these properties. The following source contains more detailed information on aggregate:

## Aggregate Sources

Aggregates can come from either natural or manufactured sources. Natural aggregates come from rock, of which there are three broad geological classifications (Roberts, et al., 1996):

**Igneous rock**

These rocks are primarily crystalline and are formed by the cooling of molten rock material beneath the earth’s crust (magma).

**Sedimentary rocks**

These rocks are formed from deposited insoluble material (e.g., the remains of existing rock deposited on the bottom of an ocean or lake). This material is transformed to rock by heat and pressure. Sedimentary rocks are layered in appearance and are further classified based on their predominant mineral as calcareous (limestone, chalk, etc.), siliceous (chert, sandstone, etc.) or argillaceous (shale, etc.).

**Metamorphic rock**

These are igneous or sedimentary rocks that have been subjected to heat and/or pressure great enough to change their mineral structure so as to be different from the original rock.

Manufactured rock typically consists of industrial byproducts such as slag (byproduct of the metallurgical processing – typically produced from processing steel, tin and copper) or specialty rock that is produced to have a particular physical characteristic not found in natural rock (such as the low density of lightweight aggregate).

## Aggregate Production

Aggregates are produced in a quarry or mine (Figure 1) whose basic function is to convert in situ rock into aggregate with specified characteristics. Usually the rock is blasted or dug from the quarry walls then reduced in size using a series of screens and crushers. Some quarries are also capable of washing the finished aggregate.

![Aggregate mine](https://pavementinteractive.org/wp-content/uploads/2008/10/Arial-mine.jpg)

*Figure 1.* Aggregate mine.

## Mineral Properties

An aggregate’s mineral composition largely determines its physical characteristics and how it behaves as a pavement material. Therefore, when selecting an aggregate source, knowledge of the quarry rock’s mineral properties can provide an excellent clue as to the suitability of the resulting aggregate. Cordon (1979) provides some general guidelines for aggregate used in HMA.

**Table 1.** Desirable Properties of Rocks for HMA (from Cordon, 1979 as referenced in Roberts et al., 1996)

| Rock Type | Hardness, Toughness | Resistance to Stripping^(1,2) | Surface Texture | Crushed Shape |
| --- | --- | --- | --- | --- |
| Igneous |  |  |  |  |
| Granite | Fair | Fair | Fair | Fair |
| Syenite | Good | Fair | Fair | Fair |
| Diorite | Good | Fair | Fair | Good |
| Basalt (trap rock) | Good | Good | Good | Good |
| Diabase (trap rock) | Good | Good | Good | Good |
| Gabbro (trap rock) | Good | Good | Good | Good |
| Sedimentary |  |  |  |  |
| Limestone | Poor | Good | Good | Fair |
| Sandstone | Fair | Good | Good | Good |
| Chert | Good | Fair | Poor | Good |
| Shale | Poor | Poor | Fair | Fair |
| Metamorphic |  |  |  |  |
| Gneiss | Fair | Fair | Good | Good |
| Schist | Fair | Fair | Good | Fair |
| Slate | Good | Fair | Fair | Fair |
| Quartzite | Good | Fair | Good | Good |
| Marble | Poor | Good | Fair | Fair |
| Serpentine | Good | Fair | Fair | Fair |
| Notes: Aggregates that are hydrophilic (water-loving) tend to strip more readily since water more easily replaces the asphalt film over each particle. Freshly crushed aggregates with many broken ionic bonds tend to strip more easily. |  |  |  |  |

In general, relationships between mineral and physical properties are quite complex, making it difficult to accurately predict how a particular aggregate source will behave based on mineral properties alone.

## Chemical Properties

While relatively unimportant for loose aggregate, aggregate chemical properties are important in a pavement material. In HMA, aggregate surface chemistry can determine how well an [asphalt cement](https://pavementinteractive.org/glossary/asphalt-cement/) binder will adhere to an aggregate surface. Poor adherence, commonly referred to as stripping, can cause premature structural failure. In PCC, aggregates containing reactive forms of silica can react expansively with the alkalis contained in the cement paste. This expansion can cause cracking, surface popouts and spalling. Note that some aggregate chemical properties can change over time, especially after the aggregate is crushed. A newly crushed aggregate may display a different affinity for water than the same aggregate that has been crushed and left in a stockpile for a year.

The following are typical chemical properties that are measured for aggregates:

- [Stripping](https://pavementinteractive.org/reference-desk/pavement-management/pavement-distresses/stripping/)
- [Alkali-Aggregate Reaction](https://pavementinteractive.org/reference-desk/pavement-management/pavement-distresses/alkali-aggregate-reaction/)

## Physical Properties

Aggregate physical properties are the most readily apparent aggregate properties and they also have the most direct effect on how an aggregate performs as either a pavement material constituent or by itself as a base or subbase material. Commonly measured physical aggregate properties are (Roberts et al., 1996):

- [Gradation and size](https://pavementinteractive.org/reference-desk/materials/aggregate/gradation/)
- [Toughness and Abrasion Resistance](https://pavementinteractive.org/reference-desk/materials/aggregate/toughness-and-abrasion-resistance/)
- [Durability and soundness](https://pavementinteractive.org/reference-desk/materials/aggregate/durability-and-soundness/)
- [Particle shape and surface texture](https://pavementinteractive.org/reference-desk/materials/aggregate/particle-shape-and-surface-texture/)
- [Cleanliness and deleterious materials](https://pavementinteractive.org/reference-desk/materials/aggregate/cleanliness-and-deleterious-materials/)
- [Moisture Content](https://pavementinteractive.org/reference-desk/materials/aggregate/moisture-content/)

These are not the only physical properties of aggregates but rather the most commonly measured. Tests used to quantify these properties are largely empirical. The physical properties of an aggregate can change over time. For instance, a newly crushed aggregate may contain more dust and thus be less receptive to binding with an [asphalt binder](https://pavementinteractive.org/glossary/asphalt-binder/)

Because aggregate makes up most of an HMA mixture, these properties largely govern how the finished pavement behaves:

- **Gradation and size.** If the largest particles are too small the mix can be unstable; if they are too large the mix is hard to work. Gradation controls how particles pack together and so the density and air voids of the mix. Dense gradations increase particle contact and reduce water infiltration while still leaving room for the binder; permeable mixes reduce the fine fraction to raise air voids. Aggregate is commonly separated into size fractions and stockpiled so that blends can be made to a target gradation.
- **Shape.** Angular particles interlock into a stronger matrix than rounded ones. Mixes with angular aggregate are harder to place and compact but resist shoving and rutting better. Crushing produces fractured, angular faces and reduces the maximum particle size. Long, thin particles tend to break during compaction, weakening the finished pavement.
- **Toughness and durability.** Aggregate must withstand stockpile loads, plant mixing and compaction before it sees traffic. In service, water trapped in particle pores can freeze and split particles, and exposed surface aggregate can be polished by traffic, reducing friction.
- **Moisture.** Water in the aggregate must be driven off at the plant, at a cost in time and fuel, because it weakens the asphalt–aggregate bond. Most moisture is held in the particles' pores, though very wet aggregate can also carry water on its surface.

Common tests for these properties include the [gradation test](https://pavementinteractive.org/reference-desk/testing/aggregate-tests/gradation-test/), [Los Angeles abrasion](https://pavementinteractive.org/reference-desk/testing/aggregate-tests/los-angeles-abrasion/), [sulfate soundness](https://pavementinteractive.org/reference-desk/testing/aggregate-tests/sulfate-soundness-test/), [percent fractured face](https://pavementinteractive.org/reference-desk/testing/aggregate-tests/percent-fractured-face-test/) and [flat and elongated particles](https://pavementinteractive.org/reference-desk/testing/aggregate-tests/flat-and-elongated-particles/) tests.

## Aggregate as Base Material

Aggregate is often used by itself as an unbound base or subbase course. When used as such, aggregate is typically characterized by the preceding physical properties as well as overall layer stiffness. Layer stiffness is characterized by the same tests used to characterize subgrade stiffness.