# AASHO Road Test

The AASHO Road Test, a $27 million (1960 dollars) investment and the largest road experiment of its time, was conceived and sponsored by the American Association of State Highway Officials (AASHO) as a study of the performance of highway…

- Canonical URL: https://pavementinteractive.org/reference-desk/design/structural-design/aasho-road-test/
- Last updated: 2018-09-19
- Review: reviewed by licensed professional engineers on the previous Pavement Interactive site, where reviewers were not recorded by name

The AASHO Road Test, a $27 million (1960 dollars) investment and the largest road experiment of its time, was conceived and sponsored by the American Association of State Highway Officials (AASHO) as a study of the performance of highway pavement structures of known thickness under moving loads of known magnitude and frequency (Highway Research Board, 1961[^1]). The test studied both [portland cement](https://pavementinteractive.org/glossary/portland-cement/) concrete and asphaltic concrete pavements, as well as certain types of short-span bridges.

The information obtained from the AASHO Road Test was crucial in advancing knowledge of pavement [structural design](https://pavementinteractive.org/reference-desk/design/structural-design/), [pavement performance](https://pavementinteractive.org/reference-desk/pavement-management/pavement-evaluation/), [load equivalencies](https://pavementinteractive.org/reference-desk/design/design-parameters/equivalent-single-axle-load/), climate effects, and much more. The basic performance information resulted in the performance equations and nomographs used in the AASHTO *Guide*. This section provides some background information on the AASHO Road Test. It should be helpful in understanding the experiment's strengths, weaknesses and limitations.

## Background

This section provides some of the basic background for the AASHO Road Test and is taken primarily from Highway Research Board's Special Report 61A, *The AASHO Road Test: History and Description of the Project* (1961).

### Location: Ottawa, Illinois

The AASHO Road Test site (which eventually became part of I-80) at Ottawa, Illinois, was typical of northern climates (Table 1).

**Table 1.** AASHO Road Test Weather

| Average Mean Temperature (July) | 24.5°C (76°F) |
| --- | --- |
| Average Mean Temperature (January) | -2.8°C (27°F) |
| Annual Average Rainfall | 837 mm (34 inches) |
| Average Depth of Frost (for fine-grained soil) | 711 mm (28 inches) |

### Time

- Construction: August 1956 - September 1958
- Test Traffic: October 1958 - November 1960
- Special Studies: Spring and early summer 1961

### Test Facilities

- Six 2-lane test loops (see Figure 1)
- Loop 1 = not subject to traffic, used to test environmental effects
- Loops 2 through 6 = subject to traffic described in Figure 2

![Loop 5 and 6 AASHO Road Test layout (redrawn from Highway Research Board, 1961 1 )](https://pavementinteractive.org/wp-content/uploads/2007/08/S_f_e21.gif)

*Figure 1.* Loop 5 and 6 AASHO Road Test layout (redrawn from Highway Research Board, 1961).

![Axle weights and distributions used on various loops of the AASHO Road Test (redrawn from Highway Research Board, 1961 1 )](https://pavementinteractive.org/wp-content/uploads/2007/08/S_f_e31.jpg)

*Figure 2.* Axle weights and distributions used on various loops of the AASHO Road Test (redrawn from Highway Research Board, 1961).

### Performance Measurements

The following measurements of performance were collected:

- [Roughness](https://pavementinteractive.org/reference-desk/pavement-management/pavement-evaluation/roughness/) and visual distress (both HMA and PCC)
- [Deflections](https://pavementinteractive.org/reference-desk/pavement-management/pavement-evaluation/deflection/), strains, etc.
- [Pavement Serviceability Index (PSI)](https://pavementinteractive.org/reference-desk/pavement-management/pavement-evaluation/present-serviceability-index/)

## HMA Pavement Materials

(Information for this section taken from Highway Research Board, 1962a and Highway Research Board, 1962b[^2])

The primary materials used in the HMA pavement sections will be briefly described below. This kind of information is helpful in comparing a particular project’s set of materials to those used at the Road Test.

### HMA

The HMA mixes used at the Road Test used:

- Crushed limestone [coarse aggregate](https://pavementinteractive.org/glossary/coarse-aggregate/)
- Natural siliceous coarse sand
- [Mineral filler](https://pavementinteractive.org/glossary/mineral-filler/) which was limestone dust
- [Penetration grade](https://pavementinteractive.org/reference-desk/materials/asphalt/penetration-grading/) [asphalt cement](https://pavementinteractive.org/glossary/asphalt-cement/) (85-100 pen)

The gradation requirements for the surface and binder courses are given in Table 2.

**Table 2.** AASHO Road Test HMA Gradation Requirements

| Sieve | Surface Course Gradation Limits | Binder Course Gradation Limits |
| --- | --- | --- |
| 1 in. | – | 100 |
| 3/4 in. | 100 | 88-100 |
| 1/2 in. | 86-100 | 55-86 |
| 3/8 in. | 70-90 | 45-72 |
| No. 4 | 45-70 | 31-50 |
| No. 10 | 30-52 | 19-35 |
| No. 20 | 22-40 | 12-26 |
| No. 40 | 16-30 | 7-20 |
| No. 80 | 9-19 | 4-12 |
| No. 200 | 3-7 | 0-6 |

For the HMA surfaced test sections (in Loops 3-6), the [surface course](https://pavementinteractive.org/glossary/surface-course/) was 1.5 inches thick. The HMA mixes were designed by the [Marshall method](https://pavementinteractive.org/reference-desk/design/mix-design/marshall-mix-design/) using 50 blows per face. The typical field asphalt contents were about 5.4 and 4.4 percent by weight of total mix for the surface and binder courses, respectively. The field [air voids](https://pavementinteractive.org/reference-desk/design/mix-design/hma-weight-volume-terms-and-relationships/) averaged 7.7 percent for the six test loops.

### Base Course

The base course material was a crushed dolomitic limestone that conformed to the gradation range shown in Table 3.

**Table 3.** AASHO Road Test Base Course Gradation Requirements

| Sieve | Specification Range Percent Passing | Actual Mean Percent Passing |
| --- | --- | --- |
| 1-1/2 in. | 010 | 100 |
| 1 in. | 80-100 | 90 |
| 3/4 in. | 70-90 | 81 |
| 1/2 in. | 60-80 | 68 |
| No. 4 | 40-60 | 48 |
| No. 10 | 28-46 | 35 |
| No. 40 | 16-33 | 20 |
| No. 100 | 7-20 | 13.5 |
| No. 200 | 3-12 | 10 |

It is significant to note that 10 percent passed the 0.075 mm (No. 200 sieve). Thus, the base was likely a bit [frost susceptible](https://pavementinteractive.org/reference-desk/design/design-parameters/frost-action/). The [CBR](https://pavementinteractive.org/reference-desk/design/design-parameters/california-bearing-ratio/) of the base material averaged 107.7 percent based on laboratory tests; however, the test results ranged from a low of 52 percent to a high of 160 percent (total of 11 tests). The minimum specified CBR was 75 percent. Typical in-place mean dry densities were about 2242 to 2275 kg/m³ (140 to 142 lb/$$ft^{3)}$$, with mean moisture contents ranging from 5.6 to 6.1 percent.

### Subbase Course

The subbase material was a sand-gravel mixture which conformed to the following gradation range shown in Table 4.

**Table 4.** AASHO Road Test Subbase Course Gradation Requirements

| Sieve | Specification Range Percent Passing | Actual Mean Percent Passing |
| --- | --- | --- |
| 1-1/2 in. | 100 | 100 |
| 1 in. | 95-100 | 100 |
| 3/4 in. | 90-100 | 96 |
| 1/2 in. | 80-100 | 90 |
| No. 4 | 55-100 | 71 |
| No. 10 | 40-80 | 52 |
| No. 40 | 10-30 | 25 |
| No. 200 | 5-9 | 6.5 |

## Sources

[^1]: Highway Research Board (1961). The AASHO Road Test: Report 1, History and Description of the Project. Special Report 61A. Highway Research Board, National Academy of Sciences. Washington, D.C.
[^2]: Highway Research Board (1962b). The AASHO Road Test: Report 5, Pavement Research. Special Report 61E. Highway Research Board, National Academy of Sciences. Washington, D.C.