# Compaction Importance

The volume of air in an HMA pavement is important because it has a profound effect on long-term pavement performance. The exact nature of that effect is nuanced, and likely not linear.

- Canonical URL: https://pavementinteractive.org/reference-desk/construction/compaction/compaction-importance/
- Last updated: 2021-07-27
- Review: reviewed by licensed professional engineers on the previous Pavement Interactive site, where reviewers were not recorded by name

The volume of air in an HMA pavement is important because it has a profound effect on long-term pavement performance. The exact nature of that effect is nuanced, and likely not linear.

- Air void content above a high-end threshold value results in a predictable reduction of pavement service life. That threshold is usually identified as 7-8%. Linden et al. (1989)[^1] stated, "The rule-of-thumb that emerges is that each 1 percent increase in air voids (over a base air void level of 7 percent) results in about a 10 percent loss in pavement life (or about 1 year less)."
- Air void content below a low-end threshold value is indicative of an unstable mixture prone to distortion and flushing. This threshold is often reported around 2-3%.

As to what happens between the high (7-8%) and low (2-3%) thresholds, there is still some uncertainty. While some assume a linear relationship between air void content and pavement life at, between, and beyond these thresholds, the true relationship may be different. Howell et al. (2021)[^2] suggest that between these thresholds (3-7% range approximately) it may be that air voids are just at an acceptable value that maximizes pavement life (with all other parameters held constant) for a typical 1/2-inch [NMAS](https://pavementinteractive.org/reference-desk/materials/aggregate/gradation-and-size/) dense-graded mixture.

Over time, the most common recommendations for acceptable air void content have been in the 3-8% range. For example, Seeds et al. (2002)[^3] concluded a good construction target was 5-6%, Cominsky et al. (1998)[^4] recommended 2-7% as a reasonable range, and Willoughby (now Schofield) and Mahoney (in 2007)[^5] and Tran et al. (in 2016)[^6] showed that a majority of states used 8% as a minimum compaction value. Further, according to Roberts et al. (1996[^7]), there is considerable evidence that dense graded mixes should not exceed 8 percent nor fall below 3 percent air voids during their service life. This is because high air void content (above 8 percent) or low air void content (below 3 percent) can cause the following [pavement distresses](https://pavementinteractive.org/glossary/pavement-distress/) (this list applies to [dense-graded HMA](https://pavementinteractive.org/reference-desk/pavement-types-and-history/pavement-types/dense-graded-hma/) and not [open-graded HMA](https://pavementinteractive.org/reference-desk/pavement-types-and-history/pavement-types/open-graded-hma/) or [SMA](https://pavementinteractive.org/reference-desk/pavement-types-and-history/pavement-types/stone-matrix-asphalt/)):

1. **Decreased stiffness and strength**. Kennedy et al. (1984[^8]) concluded that tensile strength, static and resilient moduli, and stability are reduced at high air void content.
2. **Reduced Fatigue Life**. Several researchers have reported the relationship between increased air voids and reduced fatigue life (Pell and Taylor, 1969[^9]; Epps and Monismith, 1969 [^10]; Linden et. al., 1989[^1]). Finn et al. (1973)[^11] concluded “...fatigue properties can be reduced by 30 to 40 percent for each one percent increase in air void content.” Another study concluded that a reduction in air voids from eight percent to three percent could more than double pavement fatigue life (Scherocman, 1984[^12]).
3. **Accelerated Aging/Decreased Durability**. In his Highway Research Board paper, McLeod (1967)[^13] concluded “compacting a well-designed paving mixture to low air voids retards the rate of hardening of the [asphalt binder](https://pavementinteractive.org/glossary/asphalt-binder/), and results in longer pavement life, lower pavement maintenance, and better all-around pavement performance.”
4. **[Raveling](https://pavementinteractive.org/reference-desk/pavement-management/pavement-distresses/raveling/)**. Kandhal and Koehler (1984[^14]) found that [raveling](https://pavementinteractive.org/glossary/raveling/) becomes a significant problem above about eight percent air voids and becomes a severe problem above approximately 15 percent air voids.
5. **[Rutting](https://pavementinteractive.org/reference-desk/pavement-management/pavement-distresses/rutting/)**. The amount of [rutting](https://pavementinteractive.org/glossary/rutting/) which occurs in an asphalt pavement is inversely proportional to the air void content (Scherocman, 1984[^12]). Rutting can be caused by two different mechanisms: vertical consolidation and lateral distortion. Vertical consolidation results from continued pavement compaction (reduction of air voids) by traffic after construction. Lateral distortion – shoving of the pavement material sideways and a humping-up of the [asphalt concrete](https://pavementinteractive.org/glossary/asphalt-concrete/) mixture outside the wheelpaths – is usually due to a [mix design](https://pavementinteractive.org/reference-desk/design/mix-design/) problem. Both types of rutting can occur more quickly if the HMA air void content is too low (Scherocman, 1984[^12]).
6. **[Moisture Damage](https://pavementinteractive.org/reference-desk/pavement-management/pavement-distresses/stripping/)**. Air voids in insufficiently compacted HMA are high and tend to be interconnected with each other. Numerous and interconnected air voids allow for easy water entry (Kandhal and Koehler, 1984[^14]; Cooley et al., 2002[^15]) which increases the likelihood of significant moisture damage. The [relationship between permeability, nominal maximum aggregate size and lift thickness](https://pavementinteractive.org/reference-desk/construction/compaction/permeability-vs-aggregate-size-and-lift-thickness/) is quite important and can change significantly as these parameters change.

Air voids that are either too great or too low can cause a significant reduction in pavement life. For dense graded HMA, air voids between 3 and 8 percent generally produce the best compromise of pavement strength, fatigue life, durability, raveling, rutting and moisture damage susceptibility.

## Sources

[^1]: Linden, R.N.; Mahoney, J.P. and Jackson, N.C. (1989). The Effect of Compaction on Asphalt Concrete Performance. 1989 Annual Meeting of the Transportation Research Board, Washington, D.C.
[^2]: Howell, R.; Muench, S.T.; Ashtiani, M.Z.; Feracor, J.; Russell, M. and Uhlmeyer, J. (2021). Using Large Linked Field Data Sets to Investigate Density’s Impact on the Performance of Washington State Department of Transportation Asphalt Pavements. Transportation Research Record: Journal of the Transportation Research Board. https://doi.org/10.1177/03611981211006101
[^3]: (2002). Seeds, S. B., G. R. Hicks, G. E. Elkins, H. Zhou, and T. V. Scholz. NCHRP Project 20-50(14): LTTP Data Analysis: Significance of “As-Constructed” AC Air Voids to Pavement Performance, Final Report. Transportation Research Board, Washington, D.C., 2002.
[^4]: (1998). Cominsky, R. J., B. M. Killingsworth, R. M. Anderson, D. A. Anderson, and W. W. Crockford. NCHRP Report 409: Quality Control and Acceptance of Superpave Designed Hot-Mix Asphalt. Transportation Research Board, Washington, D.C., 1998.
[^5]: (2007). Willoughby, K., and J. P. Mahoney. An Assessment of WSDOT’s Hot-Mix Asphalt Quality Control and Assurance Requirements. Report WA-RD 517.2, Washington State Department of Transportation, 2007.
[^6]: (2016). Tran, N., P. Turner, and J. Shambley. Enhanced Compaction to Improve Durability and Extend Pavement Service Life: A Literature Review. NCAT Report 16-02R, National Center for Asphalt Technol, 2016.
[^7]: Roberts, F.L., Kandhal, P.S., Brown, E.R., Lee, D.Y., and Kennedy, T.W. (1996). Hot Mix Asphalt Materials, Mixture Design, and Construction. National Asphalt Paving Association Education Foundation. Lanham, MD.
[^8]: Kennedy, T.W.; Roberts, F.L.; and McGennis, R.B. (1984). “Effects of Compaction Temperature and Effort on the Engineering Properties of Asphalt Concrete Mixtures.” Placement and Compaction of Asphalt Mixtures, F.T. Wagner, Ed. ASTM Special Technical Publication 829. American Society for Testing and Materials, Philadelphia, PA. pp. 48-66.
[^9]: Pell, P.S. and Taylor, I.F. (1969). “Asphalt Road Materials in Fatigue.” Proceedings of the Association of Asphalt Paving Technologists, Vol. 38. pp. 371-464.
[^10]: Epps, Jon A. and Monismith, Carl L. (1969). “Influences of Mixture Variables on the Flexural Fatigue Properties of Asphalt Concrete.” Proceedings of the Association of Asphalt Paving Technologists, Vol. 38. pp. 423-464.
[^11]: Finn, F.N.; Nair, K.; and Hilliard, J. (1973). Minimizing Premature Cracking of Asphalt Concrete Pavements. National Cooperative Highway Research Program Project 9-4. Transportation Research Board, National Research Council. Washington, D.C.
[^12]: Scherocman, J.A. (1984). Guidelines for Compacting Asphalt Concrete Pavement. Better Roads, Vol. 54, No. 3. pp. 12-17.
[^13]: McLeod, N.W. (1967). “Influence of Viscosity of Asphalt-Cements on Compaction of Paving Mixtures in the Field.” Highway Research Record No. 158: Bituminous Concrete Mixes: 6 Reports. Highway Research Board, National Research Council, Washington, D.C.
[^14]: Kandhal, P.S. and Koehler, W.C. (1984). Pennsylvania’s Experience in the Compaction of Asphalt Pavements. Placement and Compaction of Asphalt Mixtures, F.T. Wagner, Ed. ASTM Special Technical Publication 829. American Society for Testing and Materials. Philadelphia, PA. pp. 93-106.
[^15]: Cooley, L.A.; Prowell, B.D. and Brown, E.R. (2002). Issues Pertaining to the Permeability Characteristics of Coarse-Graded Superpave Mixes. NCAT Report No. 02-06. National Center for Asphalt Technology. Auburn, AL. https://web.archive.org/web/20081010144810/http://www.eng.auburn.edu/center/ncat/reports/rep02-06.pdf